HLM-107
This specification describes the 107-type lithium-ion battery cathode material produced by Hunan Haili Lithium Technology Co., Ltd. (hereinafter referred to as Haili Lithium), with the molecular formula LiMn2O4.
classification:
Lithium battery
keyword:
haili
annex:
Contact Us
DESCRIPTION
1 Introduction
This specification describes the 107-type lithium-ion battery cathode material produced by Hunan Haili Lithium Technology Co., Ltd. (hereinafter referred to as Haili Lithium), with the molecular formula LiMn2O4.
2. Model: HLM-107
3. Scope of application of the product
This product is suitable for mid-end small power products, such as low-speed electric vehicles, electric bicycles, small energy storage, large energy storage and other fields.
4. Product Features
This product adopts metal element compound doping technology to optimize the cycle performance and cost performance of lithium manganate. This material has good processing performance, excellent cycle performance, high cost performance and good consistency.
(1) The product particles are complete and regular spinel phase, the particle size distribution is uniform, and the material processing performance is superior.
(2) The comprehensive performance of the product is excellent. The normal temperature 1C gram capacity is greater than 105mAh/g, the cycle is 500 cycles, and the capacity retention rate is greater than 80%.
(3) There is no impurity phase in X-ray diffraction of the product.
5. Physical indicators:
5.1. Physical and chemical indicators
product name |
Lithium manganese oxide |
model |
HLM-107 |
|
Chemical Composition and Physical Indicators |
||||
Analysis Project |
standard value |
typical value |
testing method |
|
Mn,% |
≥57.0 |
58.85 |
volumetric method |
|
Li,% |
4.2±0.2 |
4.18 |
AAS |
|
K,% |
≤0.05 |
0.004 |
AAS |
|
That,% |
≤0.35 |
0.1792 |
AAS |
|
Fe,% |
≤0.01 |
0.0032 |
AAS |
|
That,% |
≤0.05 |
0.0189 |
AAS |
|
With,% |
≤0.01 |
0.0011 |
AAS |
|
SO42-,% |
≤1.5 |
1.13 |
gravimetric method |
|
H 2 O, % |
≤0.08 |
0.03 |
Karl Fischer method |
|
Specific surface, m 2 /g |
≤1.0 |
0.68 |
Specific surface tester |
|
Magnetic substance, ppb |
≤3500 |
3431 |
ICP |
|
Tap density, g/ cm3 |
≥1.8 |
2.09 |
Tap Density Meter |
|
Granularity (um) (can be adjusted according to customer requirements) |
D10 |
≥3.0 |
3.82 |
Malvern particle size analyzer |
D50 |
13~18 |
16.3 |
||
D90 |
≤40 |
31.9 |
5.2. Basic electrical performance indicators
project |
standard value |
typical value |
testing method |
Compacted density (g/cm 3 ) |
≥2.8 |
2.9 |
Reference data provided by downstream customers |
Button power 1C discharge specific capacity (mAh/g) |
≥105 |
110 |
Blue Electric Battery Tester |
500-cycle cycle capacity retention at room temperature (1C charge and discharge) |
≥80 |
84 |
Blue Electric Battery Tester |
(Remarks: The relevant electrical performance data in this table are provided by the battery manufacturer for reference only, and the quality of the product is subject to the quality inspection sheet.)
5.3. Particle size distribution
5.4 Electron microscope image
6. Packaging and storage conditions
6.1. Packing method: Inner aluminum foil bag, vacuum packaging, outer carton, 25kg/box.
6.2. Requirements for stacking layers: carton packaging ≤ 3 layers.
6.3. Label style: the default Haili lithium battery shipping label, if the customer has special requirements, it can be implemented according to the label style provided by the customer.
6.4. Storage conditions: Keep sealed and avoid direct sunlight. The recommended storage temperature is ≤37°C and the humidity is ≤50%RH. The shelf life is 1 year. If the product exceeds the shelf life, it should be inspected by our company and re-evaluated whether it can be used normally.
6.5. Under the condition of unsealing, strictly control the storage humidity to ≤30%RH, and use it as soon as possible.
7. Precautions for transportation
When loading, do not place heavy objects on top of the cartons to prevent deformation of the cartons; prevent extrusion and sun and rain; use vehicles, trains, ships, planes and other vehicles for transportation.
8. Suggestions for processing and use
Positive electrode ratio: lithium manganate 94.5%~96.0%, conductive agent 1.0%~2.5%, PVDF 2.0%~3.0%. It is recommended to use PVDF with a molecular weight greater than 1 million as the binder. If the binder is made by the suspension method, the dosage can be adjusted to 1.5% to 2.0%.
Suggested negative electrode excess ratio: 8﹪~12﹪.
It is recommended to use compaction: 2.80~2.90g/cm3.
Recommended